TEROSON 5510

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

TEROSON 5510

Main features

  • Elastic Modified-Silane Bonding
  • Fast Skin-Over Processing
  • 2 mm Depth of Cure

Product Description

TEROSON® MS 5510™ BLACK is a one-component, moisture-curing modified silane polymer adhesive and sealant for elastic bonding and sealing across a range of substrates. The black homogeneous paste cures by reaction with atmospheric moisture to form an elastomeric thermoset material. It combines high strength, high elongation, high initial tack, sag resistance, and compatibility with suitable paint systems for interior and exterior applications.

Key features

  • Elastic bonding and sealing: Delivers a flexible cured bond with high elongation for joints subject to movement.
  • Moisture-curing, one-component system: Requires no mixing and develops functional strength in approximately 24 hours under normal conditions.
  • Application-friendly formulation: Sag resistant, high in initial tack, compatible with suitable paint systems, and free of solvents, isocyanates, silicones, and PVC.
Product Family

TEROSON 5510

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Appearance
Black homogeneous paste
Specific Gravity
1.4 - 1.5
Physical Properties
Viscosity
150,000 to 240,000 mPa.s
Mechanical Properties
Elongation
376 %
Thermal Properties
Glass Transition Temperature (Tg)
-69 °C

Additional Information

Technical properties

As-supplied / before-processing properties

Typical properties of the uncured material; values are reference data rather than guaranteed product specifications.

Property Value Unit Method / condition
Technology Flextec™ polymer — Uncured material
Chemical type Modified silane polymer — Uncured material
Appearance Black homogeneous paste — Uncured material
Components One component — No mixing required
Specific gravity 1.4–1.5 — At 25°C
Extrusion rate 150–600 g/min Typical uncured-material property
Flow ≤2.5 mm ISO 7390
Viscosity 150,000–240,000 mPa·s Cone and plate, 25°C; shear rate 10 s−1
Skin-over time 20–50 min 25 ± 2°C, 50 ± 5% RH
Flash point >93 °C ASTM D3278, Setaflash closed cup; SDS value
Technical properties

After-processing / final-state properties

Typical cured-material properties depend on the stated cure schedule, substrate, specimen, and test method.

Property Value Unit Method / condition
Depth of cure ≥2 mm After 24 hours
Shore hardness 35–50 Shore A ISO 868; cured 7 days at 22°C and 50 ± 5% RH
Tensile strength ≥1.5 N/mm² ISO 527-3; cured 7 days at 22°C and 50 ± 5% RH
Elongation at break 376 % ISO 527-3; cured 21 days at 22°C and 50 ± 5% RH
Glass-transition temperature −69 °C ISO 11357-2; cured 21 days at 22°C and 50 ± 5% RH
Nonvolatile content 98 % ASTM D2369; cured 21 days at 22°C and 50 ± 5% RH
Lap-shear strength 1.6 N/mm² ISO 4587; grit-blasted steel; cured 21 days at 22°C
Lap-shear strength 1.7 N/mm² ISO 4587; glass; cured 21 days at 22°C
T-peel strength 0.2 N/mm ISO 11339; aluminum; cured 21 days at 22°C
Impact strength 2.7 J ISO 9653; aluminum; cured 21 days at 22°C

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers