MP 54110

Harmonization Code : 3214.10.00 | Putty and other mastics | Resin cements, caulking compounds and other mastics

MP 54110 MP 54110

Main features

  • 1:1 Meter-Mix Dispensing
  • 30-60 Minute Handling Cure
  • 15.9 MPa Aluminum Shear

Product Description

H.B. Fuller MP54110 Epoxy Adhesive uses a clear, two-part unfilled epoxy system to bond metals, ceramics, and most plastics. The liquid components mix 1:1 by weight or volume and produce a typical mixed viscosity of 20,000 cP for cartridge and meter-mix-dispense application. At 25 deg C, a 20 g batch has an 8-12 minute pot life. Assemblies reach handling cure in 30-60 minutes and full cure in 24 hours at room temperature. The cured adhesive has Shore D 80 hardness, 10% elongation, and a typical operating range of -40 to 130 deg C.

Key features

  • One-to-one mix ratio: Mixes 1:1 by weight or volume for cartridge or meter-mix-dispense application.
  • Rapid handling cure: Reaches handling cure in 30-60 minutes at room temperature.
  • Aluminum overlap shear: Provides 15.9 MPa typical overlap shear on acid-etched aluminum under ASTM D1002 conditions.

Applications / Suitable for

  • Bonding metal and ceramic assemblies
  • Bonding most plastic assemblies
  • Cartridge or meter-mix-dispense application
Product Family

MP 54110

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Appearance
Clear
Chemistry Type
Epoxy
Component System
two component

Additional Information

Technical properties

Uncured and working properties

Property Value Unit Method / condition
Appearance Clear liquid As supplied
Mix ratio 1:1 by weight or volume Resin to hardener
Mixed viscosity 20,000 cP Typical
Mixed specific gravity 1.16 Typical
Pot life 8-12 min 20 g mass at 25 deg C
Storage temperature 12-25 deg C Unopened containers
Technical properties

Cured properties

Property Value Unit Method / condition
Shore hardness 80 Shore D ASTM D2240
Operating temperature -40 to 130 deg C Typical range
Overlap shear 15.9 MPa ASTM D1002; acid-etched aluminum; 25 deg C; 50% RH
Elongation 10 % Cured adhesive

Leading Brands Trust in Our Products and Services