LORD 363

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LORD 363

Main features

  • 3 to 5-Minute Working Window
  • Self-Leveling Flowable Placement
  • Solvent-Free Bonding Formulation

Product Description

LORD® 363-A/363-B Epoxy Adhesive is a fast-setting, two-component epoxy adhesive designed to bond scuffed sheet molding compounds (SMC), wood, fiberglass reinforced plastics (FRP) and other supported plastics. Its self-leveling consistency flows into hard-to-reach areas and supports assemblies with tight tolerances. The solvent-free system can be cured at room temperature or with heat for faster processing.

Key Features

  • Fast room-temperature cure with a 3–5 minute working time and handling strength in 15–30 minutes.
  • Self-leveling consistency for flowing into hard-to-reach areas and bonding close-fitting parts.
  • Solvent-free formulation that is nonflammable and virtually odorless.
  • Room-temperature or heat curing to support different production requirements.

Applications / Suitable for

  • Scuffed sheet molding compound bonding
  • Fiberglass reinforced plastic bonding
  • Wood and supported plastic assemblies
  • Close-fitting parts and hard-to-reach bond areas
Product Family

LORD 363

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Appearance
363A Resin: Clear Liq | 363B Hardener: Light Amber Liq
Density
Resin: 1126 -1198 | Hardener: 1114 -1150 kg/m3
Physical Properties
Viscosity
Resin: 7000 -16,000 | Hardener: 8000 - 20,000 mPa.s
Thermal Properties
Flash Point
Resin: >93 | Hardener: >93 °C

Additional Information

Technical Properties

As-Supplied / Before-Processing Properties

Typical component and mixed properties. Values are typical and are not intended for specification purposes.

Property 363-A Resin 363-B Hardener Mixed Method / Condition
Appearance Clear liquid Light amber liquid Light amber liquid Typical
Viscosity 7,000–16,000 cP 8,000–20,000 cP — Brookfield HAT, 10 rpm at 77°F (25°C); Spindle 4 for resin and T-C spindle for hardener
Density 9.4–10.0 lb/gal
(1126–1198 kg/m³)
9.3–9.6 lb/gal
(1114–1150 kg/m³)
— Typical
Flash Point >200°F
(>93°C)
>200°F
(>93°C)
— Closed cup
Mix Ratio 1 part 1 part 1:1 Resin to hardener, by volume
Solids Content — — 100% Mixed adhesive
Working Time — — 3–5 minutes 54 g mass at 75°F (24°C)
Time to Handling Strength — — 15–30 minutes Typical
Shelf Life 2 years 2 years — From date of manufacture; store at 60–80°F (16–27°C) in original, unopened containers
Technical Properties

After-Processing / Final-State Properties

Supported cure and final-state characteristics. Values are typical and are not intended for specification purposes.

Property Value Unit Method / Condition
Cure to Full Strength 4–6 hours Adhesive, substrates and ambient temperature at 65°F (18°C) or higher
Maximum Bondline Temperature During Heat Cure 325
(162)
°F
(°C)
Higher temperatures accelerate cure; firm cure recommendations depend on material composition and heating method
Cured Appearance Tan — Typical

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers