LOCTITE EA E-20NS

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA E-20NS

Main features

  • Non-Sag Vertical Bonding
  • Tough High-Peel/Shear Bonding
  • Electrically Insulating Multi-Material Bonding

Product Description

LOCTITE® EA E-20NS™ is a two-component, industrial-grade epoxy adhesive that cures at room temperature to form an off-white, tough bondline. Its non-sagging, medium-viscosity formulation supports controlled application on vertical surfaces while reducing run-off. The adhesive develops strong bonds on aluminum, stainless steel and other metals, as well as glass, ceramics and selected plastics. It has a 20-minute working life and provides high peel resistance, high shear strength and electrical insulation after full cure. The cured material also resists a range of chemicals and solvents.

Key features

  • Non-sagging consistency: Supports application on vertical surfaces without excessive run-off.
  • Tough bonded joints: The cured epoxy provides high peel resistance and high shear strength.
  • Electrical insulation: Fully cured material has a typical dielectric breakdown strength of 24 kV/mm.

Applications / Suitable for

  • Bonding aluminum, stainless steel and other metals
  • Bonding glass and ceramics
  • Bonding compatible plastics
  • Vertical-surface bonding where non-sag application is required
Product Family

LOCTITE EA E-20NS

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
Off white
Mix Ratio
2:1
Physical Properties
Viscosity (Part A)
80,000-280,000 mPa.s
Viscosity (Part B)
30,000-90,000 mPa.s
Mechanical Properties
Elongation
4 %
Electrical Properties
Dielectric Strength
24 kV/mm

Additional Information

Technical properties

As-supplied / before-processing properties

Typical properties of the separate resin and hardener components and the material after mixing.

Property Value Unit Method / condition
Mix ratio, resin to hardener 2:1 By volume Two-component system
Mix ratio, resin to hardener 100:48 By weight Two-component system
Resin viscosity 80,000–280,000 mPa·s (cP) Brookfield RVT, 25 °C, spindle 7, 20 rpm
Hardener viscosity 30,000–90,000 mPa·s (cP) Brookfield RVT, 25 °C, spindle 7, 50 rpm
Mixed specific gravity 1.43 — At 25 °C
Working life 20 min Mixed material
Tack-free time 20 min Mixed material
Mixed appearance Off-white — After resin and hardener are mixed

After-processing / final-state properties

Typical physical, electrical and adhesive properties after curing under the stated conditions.

Property Value Unit Method / condition
Glass transition temperature 75 °C Cured at 25 °C
Coefficient of thermal expansion 52 × 10−6 pre-Tg; 183 × 10−6 post-Tg K−1 ISO 11359-2; cured at 25 °C
Shore hardness 84–94 Shore D ISO 868; cured at 25 °C
Elongation 4 % ISO 527-2; cured at 25 °C
Tensile strength 23 N/mm² ISO 527-2; cured at 25 °C
Dielectric breakdown strength 24 kV/mm IEC 60243-1; cured at 25 °C
Lap shear strength on grit-blasted steel 19.2 N/mm² Cured 5 days at 22 °C
Lap shear strength on acid-etched and abraded aluminum 17.3 N/mm² Cured 5 days at 22 °C; 0.1–0.2 mm bondline gap