LOCTITE E-214HP

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE E-214HP

Main features

  • One-Component Adhesive System
  • Heat-Activated Bonding Cure
  • Thermal Shock Resistance

Product Description

LOCTITE® EA E-214HP™ is a one-component, heat-curing epoxy adhesive designed for high-strength structural bonding applications. This thixotropic, no-mix formulation develops tough, durable bonds with outstanding peel resistance, impact strength, thermal shock resistance, and excellent electrical and mechanical properties. Once fully cured, it offers broad chemical resistance and bonds effectively to metals, glass, ceramics, and engineering plastics.

Key Features & Benefits

  • One-component epoxy requiring no mixing.
  • Heat-activated cure for high-performance structural bonding.
  • Excellent peel resistance and impact strength.
  • Outstanding thermal shock resistance.
  • Excellent mechanical and electrical properties.
  • Resistant to a wide range of chemicals and solvents.
  • Bonds metals, glass, ceramics and plastics.

Recommended Applications

  • Structural metal bonding.
  • Glass and ceramic assembly.
  • Engineering plastic bonding.
  • Industrial equipment manufacturing.
  • High-temperature structural adhesive applications.
Product Family

LOCTITE E-214HP

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Appearance
Light grey paste
Specific Gravity
1.11
Physical Properties
Viscosity
2,000,000 - 3,000,000 mPa.s
Thermal Properties
Glass Transition Temperature (Tg)
120 °C
Mechanical Properties
Elongation
7 %

Additional Information

Technical Properties

As-Supplied / Before-Processing Properties

Property Value Unit Condition
Technology Epoxy — One-component adhesive
Appearance Light Grey Paste — As supplied
Specific Gravity 1.11 — 25°C
Brookfield Viscosity 2,000,000 - 3,000,000 mPa·s (cP) Spindle 7, 1 rpm
Brookfield Viscosity 1,500,000 mPa·s (cP) Spindle 7, 2.5 rpm
Physical Form Thixotropic Paste — Ready-to-use
Storage Temperature < 4 °C Recommended storage
Technical Properties

After-Processing / Final-State Properties

Property Value Unit Condition / Method
Glass Transition Temperature (Tg) 120 °C ISO 11359-2
Shore Hardness 85 Shore D ISO 868
Elongation at Break 7 % ISO 527-2
Tensile Strength 31 N/mm² ISO 527-2
Dielectric Breakdown Strength 22 kV/mm IEC 60243-1
Lap Shear Strength (Steel) 33 N/mm² 2 h @ 120°C + 4 h @ 22°C
Lap Shear Strength (Aluminum) ≥13.8 N/mm² Acid etched & abraded
Lap Shear Strength (Stainless Steel) 37 N/mm² Structural bond
Block Shear Strength (Glass) 23 N/mm² ISO 13445
Recommended Cure Schedule 2 h @ 120°C — 150°C cure maximizes properties

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers