LOCTITE 4210

Harmonization Code : 3824.99.92.97 | Prepared binders for foundry molds or cores; chemical products and preparations of the chemical or allied industries (including those consisting of mixtures of natural products), not elsewhere specified or included: other : other : other

LOCTITE 4210

Main features

  • Elastomer-Toughened Impact Resistance
  • Low-Viscosity Thin-Gap Bonding
  • Fast Multi-Substrate Fixturing

Product Description

LOCTITE 4210 is a black, low-viscosity, elastomer-toughened ethyl cyanoacrylate instant adhesive for bonding metals, plastics, and rubbers. The one-part liquid cures with atmospheric moisture and requires no mixing. Its toughened formulation adds impact and peel strength while improving resistance to heat and humidity. A Brookfield viscosity of 110 to 210 mPa s supports controlled flow into thin bond areas, and fixture time ranges from seconds to several minutes depending on substrate. The adhesive performs best in bond gaps around 0.05 mm and develops full chemical and solvent resistance after at least 24 hours.

Key features

  • Elastomer-toughened performance: The formulation adds impact and peel strength with improved heat and humidity resistance.
  • Low-viscosity one-part flow: A 110 to 210 mPa s viscosity supports controlled application in thin bond areas without mixing.
  • Substrate-dependent rapid fixture: Documented fixture times range from 5 seconds on nitrile rubber to 150 seconds on degreased steel.

Applications / Suitable for

  • Thin-gap bonding of metals
  • Bonding supported plastics and rubbers
  • Assemblies requiring improved peel, impact, heat, or humidity resistance
Product Family

LOCTITE 4210

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Chemistry Type
Ethyl cyanoacrylate
Color
Black liquid
Component System
One component
Specific Gravity
1.05
Thermal Properties
Glass Transition Temperature (Tg)
165 °C
Linear thermal expansion
80×10^-6 K -1
Thermal Conductivity
0.1 W/m.K
Physical Properties
Viscosity
110 to 210 mPa.s
Electrical Properties
Dielectric Strength
28 kV/mm
Surface Resistivity
10×10^15 Ohms/sq
Volume Resistivity
10×10^15 Ohms⋅cm
Curing Conditions
Fixture Time
90 -150 seconds

Additional Information

Technical properties

As-supplied / before-processing properties

Typical values for the product before cure, application, or assembly.

PropertyValueUnitMethod / condition
AppearanceBlack liquid-Uncured
Chemical typeEthyl cyanoacrylate-As supplied
ComponentsOne part-No mixing required
Specific gravity1.05-25 deg C
Viscosity110 to 210mPa sBrookfield HBT, spindle 3, 50 rpm, 25 deg C
Cure mechanismHumidity-Atmospheric moisture
Optimal storage2 to 8deg CUnopened container in a dry location
Technical properties

After-processing / final-state properties

Typical values for the cured or installed product under the listed conditions.

PropertyValueUnitMethod / condition
Fixture time, degreased steel90 to 150s22 deg C, 50% RH; time to 0.1 N/mm^2 shear strength
Fixture time, aluminum20 to 50s22 deg C, 50% RH; time to 0.1 N/mm^2 shear strength
Fixture time, nitrile rubber5 to 10s22 deg C, 50% RH; time to 0.1 N/mm^2 shear strength
Glass transition temperature165deg CASTM E 228; after 24 h at 22 deg C
Lap shear strength, grit-blasted steel23 to 27N/mm^2ISO 4587; cured 24 h at 22 deg C
Dielectric breakdown strength28kV/mmIEC 60243-1; after 24 h at 22 deg C

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers