LOCTITE 1C

Harmonization Code : 2901.10.00.00 | Acyclic hydrocarbons; Saturated

LOCTITE 1C LOCTITE 1C

Main features

  • Controlled Two-Part Mixing
  • Flexible Cure Scheduling
  • Machinable Cured Epoxy

Product Description

LOCTITE EA 1C is a two-part epoxy adhesive and sealant supplied as resin and hardener for bonding, sealing, and repair work. The off-white mixture cures at room temperature after mixing and can also be heat cured when a shorter process is required. A 2.5:1 volume mix ratio and at least 20 minutes of pot life at 25 deg C support controlled preparation and placement. After cure, the material can be machined or sanded, and the cured state is characterized by thermal, dielectric, and mechanical properties. It is suited to assemblies involving metals, many plastics, and wood where a durable epoxy bond or sealed repair is required.

Key features

  • Controlled two-part mixing: A 2.5:1 resin-to-hardener volume ratio supports repeatable preparation.
  • Flexible cure scheduling: The mixed epoxy cures at room temperature or with documented heat-cure schedules.
  • Machinable cured material: The cured epoxy can be machined and sanded for finished repairs and assemblies.

Applications / Suitable for

  • Bonding and sealing metals
  • Repairing many plastics and wood
  • General-purpose epoxy adhesive and sealant assemblies

Technical Specifications

General Properties
Appearance
Off-White
Chemistry Type
Epoxy
Component System
2
Mix Ratio
A/B: 2.5/1
Pot Life
≥20 minutes
Solids
100 %
Specific Gravity
A/B: 1.63/1.66
Physical Properties
Viscosity (Part B)
500,000 to 900,000 mPa.s
Electrical Properties
Dielectric Strength
23.1 kV/mm

Additional Information

Technical properties

As-supplied / before-processing properties

Typical values for the product before cure or assembly.

PropertyValueUnitMethod / condition
Resin appearanceOff-white-Part A, uncured
Hardener appearanceGreen-Part B, uncured
Mix ratio2.5:1volumeResin:hardener
Mix ratio100:44weightResin:hardener
Resin viscosity120,000 to 350,000mPa sBrookfield RV, spindle 7, 10 rpm, 25 deg C
Hardener viscosity500,000 to 900,000mPa sBrookfield RV, spindle 7, 2 rpm, 25 deg C
Pot life>=20min100 g mixed mass at 25 deg C
Technical properties

After-processing / final-state properties

Typical values for the cured product under the listed conditions.

PropertyValueUnitMethod / condition
Handling strength3 to 4hCured at 25 deg C
Complete room-temperature cure72hCured at 25 deg C
Shore hardness>=65Shore DCured 2 h at 60 deg C
Glass transition temperature87deg CCured 3 h at 120 deg C
Thermal conductivity0.77W/(m K)ASTM E1530; cured 3 days at 25 deg C; tested at 100 deg C
Lap shear strength18.7N/mm^2Etched aluminum; cured 2 h at 60 deg C; tested at 25 deg C
Dielectric breakdown strength23.1kV/mmCured 3 days at 25 deg C