BCP-1509 | Medium voltage Busbar Coating Powder

Harmonization Code : 3907.30.00.85 | Polyacetals, other polyethers and epoxide resins, in primary forms; polycarbonates, alkyd resins, polyallyl esters and other polyesters, in primary forms : Epoxide resins : Other

BCP-1509 | High voltage Busbar Coating Powder

Main features

  • Reddish Brown Color
  • Up to 3mm thickness
  • RTI Class B

Product Description

LINQSOL BCP-1509 is a Reddish brown, busbar epoxy coating powder. It aims at medium to high voltage busbar applications. It performs uniform and smooth coating results from 0.3mm to 3mm.

It is especially suitable for large busbar applications used for power distribution. With optimized gel time and flow, it allows large busbars with high heat capacity dip multiple times in fluidized bed to build thickness as high as 3mm without dripping and sag. BCP-1509 meets the UL 746B Relative Thermal Index (RTI) of 105°C and CTI 600V.  For small busbar applications, we recommend BCP-1507 with powder quick build rate. 

Features:

  • Aims at medium to high voltage application
  • Comparable with DK19
  • Good adhesion to copper, alumina 
  • Thick and no-sag coating performance
  • Both electrostatic spray and fluidized bed coating

Recommended coating Temperature:

  • 180 – 230 °C. (200 °C x 30 min)
Product Family

LINQ BCP-1509

1. Select Package Type
Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

Product availability
US Shipping in 8 weeks
CA Shipping in 8 weeks
EU Shipping in 8 weeks
Packaging
Please select Package Type.
TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
Reddish Brown
Process Method
Fluidized bed, electrostatic spray
Specific Gravity
1.5
Thermal Properties
Glass Plate Flow
18 mm
UL 94 Rating
V-0
Electrical Properties
Breakdown Voltage
35 V
Volume Resistivity
0.0000000000001 Ohms⋅cm
Other Properties
RoHS Compliant
YES
Mechanical Properties
Edge Coverage
45 %
Impact Strength
500 mm

Additional Information

 

BCP-1509 Fluidized Bed Coating Performance 
Preheat Temperature Dip Times Minimum Coat Thickness Breakdown Voltage Pass
200°C 1 0.35 mm >20 kV
200°C 4 0.60 mm >20 kV
240°C 4 0.75 mm >20 kV
240°C 7 1.10 mm  >20 kV

Busbar for testing: Aluminum strip (75mm x 50mm x 5mm)

Breakdown volatge test: DC holiday detector

OBSERVATION

  • Coating appearance: Smooth, no-sag, no-dripping, great edge coverage
  • Coating process: Quick build rate on thickness
  • Suitable thickness: both thin and thick thickness (>1mm)

DISCUSSION

BCP-1509 presents excellent coating performance. BCP-1509 is developed based on BCP-1507 with slightly lower flowability while melting, thus has less chance to drip or sag with multiple dipping times.  It is designed to coat more than 3mm on large size busbars or copper busbars.

BCP-1509 Powder In Fluidized Bed

Storage

Store in a ventilated, dry, and clean environment below 25°C. Keep away from fire and heat sources. It is strictly forbidden to store in outdoor environments. At proper storage conditions, the product has a shelf life of 6 months.

Precautions

  • Avoid long-term skin contact. Powder that touched the skin should be rinsed off quickly.
  • During operation dust-proof masks should be used to avoid inhalation.
  • Keep the oven temperature stable, so as not to affect the colour and quality of the coating due to excessive temperature deviation.
  • The concentration of dust should be controlled within a safe range to avoid malfunction of the coating equipment.

Linqsol Busbar Coating Products Selection Guide

  BCP-1000 BCP-1504 BCP-1507 BCP-1509
Specific Gravity, g/cc 1.45±0.05 1.52±0.05 1.50 1.50
Glass Plate Flow 18-22mm@150°C, 45° 10-22mm@150°C, 60° 19-20 mm@180°C 19-20 mm@180°C
Hot Plate Gel Time 70 sec@150°C 45±15 sec@160°C 60 sec@180°C 60 sec@180°C
Edge Coverage, % 45 45 45 45
Hardness, shore D >80 >90 - -
Impact Resistance, cm >50 >50 >50 >50
Dielectric Strength (kV/mm) >42 >35 >35 >35
Flammability, UL94 V-0 V-0 V-0 V-0
Min. Coating Thickness 0.3mm 0.3mm 0.1mm 0.3mm
Max. Coating Thickness 1mm 1mm 2mm 3mm
Electrostatic Spray ■■■ ■□□ ■■■ ■■■
Dip Coating ■□□ ■■■ ■■■ ■■■
Available Color

●●●●●

●●

●●●●●

●

Preheat Temperature 180~240 °C 150~180 °C 180~230 °C 180~230 °C
Curing Conditions 200°C x 15min 200°C x 15min 200°C x 30min 200°C x 30min

Leading Brands Trust in Our Products and Services