BCP-1507 | Medium voltage Busbar Coating Powder

Harmonization Code : 3907.30.00.85 | Polyacetals, other polyethers and epoxide resins, in primary forms; polycarbonates, alkyd resins, polyallyl esters and other polyesters, in primary forms : Epoxide resins : Other

BCP-1507 | Medium voltage Busbar Coating Powder

Main features

  • Multiple colors
  • All around usage
  • RTI Class A

Product Description

LINQSOL BCP-1507 with its optimized gel time and flow ,builds up quickly and performs excellent coating results. With a wide coating thickness range of 0.1 ~ 2.0 mm, it could be used for both low (600V) and medium-voltage (38kV) busbar applications. Colors are available in orange (RAL2003), red, black (RAL9005), blue and green. 

It is especially suitable for EV busbars and small busbars applications. The low heat capacity of small busbars limit the dipping times, thus it requires coating powders low pick-up temperature and high build rate, which BCP-1507 aims at. BCP-1507 meets the UL 746B Relative Thermal Index (RTI) of 105°C and CTI 600V.  For large busbar applications, we recommend BCP-1509. 

Key Features:

  • One-powder solution from low to medium voltage
  • Comparable with DK15-0606/DK15-0907
  • Good adhesion to copper, alumina 
  • Good flowability and low viscosity while melting
  • Low pick up temperature 
  • High powder build rate (able to reach 0.5mm with 1 dip)
  • Both electrostatic spray and fluidized bed coating

Recommended coating Temperature:

  • 180 – 230 °C. (200 °C x 30 min)

Additional Information:

  • Linqsol busbar coating products selection guide
  • BCP-1507 coating test results
Product Family

LINQ BCP-1507

1. Select Package Type
Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

Product availability
US Shipping in 8 weeks
CA Shipping in 8 weeks
EU Shipping in 8 weeks
Packaging
Please select Package Type.
TDS, SDS & Technical Documents

Technical Specifications

Thermal Properties
Glass Plate Flow
20 mm
UL 94 Rating
V-0
Electrical Properties
Breakdown Voltage
35,000 V
Volume Resistivity
0.0000000000001 Ohms⋅cm
General Properties
Color
Orange
Process Method
Fluidized bed, electrostatic spray
Specific Gravity
1.5
Other Properties
RoHS Compliant
YES
Mechanical Properties
Edge Coverage
45 %
Impact Strength
500 mm

Additional Information

 

BCP-1507 Fluidized Bed Coating Performance 
Preheat Temperature Dip Times Minimum Coat Thickness Breakdown Voltage Pass
200°C 1 0.43 mm >20 kV
240°C 1 0.43 mm >20 kV
240°C 2 0.48 mm >20 kV
240°C 3 0.70 mm  >20 kV
240°C 4 0.85 mm  >20 kV
240°C 8 1.30 mm  >20 kV

Busbar for testing: Aluminum strip (75mm x 50mm x 5mm)

Breakdown volatge test: DC holiday detector

OBSERVATION

  • Coating appearance: Smooth, no-sag, no-dripping, great edge coverage
  • Coating process: Quick build rate on thickness
  • Suitable thickness: both thin and thick thickness (>1mm)

DISCUSSION

BCP-1507 presents excellent coating performance with dielectric strength. It is highly potential to coat more than 2mm on large size busbars or copper busbars.

 

 

Storage

Store in a ventilated, dry, and clean environment below 25°C. Keep away from fire and heat sources. It is strictly forbidden to store in outdoor environments. At proper storage conditions, the product has a shelf life of 6 months.

Precautions

  • Avoid long-term skin contact. Powder that touched the skin should be rinsed off quickly.
  • During operation dust-proof masks should be used to avoid inhalation.
  • Keep the oven temperature stable, so as not to affect the colour and quality of the coating due to excessive temperature deviation.
  • The concentration of dust should be controlled within a safe range to avoid malfunction of the coating equipment.

Linqsol Busbar Coating Products Selection Guide

  BCP-1000 BCP-1504 BCP-1507 BCP-1509
Particle size

>320 mesh, 20.5%

180-230 mesh, 74%

100-180 mesh, 5.5%

<100 mesh, 0%

>400 mesh, 15~30%

140-400 mesh, 44~73%

100-140 mesh, 10~20%

<100 mesh, 2~6%

>320 mesh, 10%

<80 mesh, 0%

>320 mesh, 10%

<80 mesh, 0%

Specific Gravity, g/cc 1.45±0.05 1.52±0.05 1.50 1.50
Glass Plate Flow 18-22mm@150°C, 45° 10-22mm@150°C, 60° 19-20 mm@180°C 19-20 mm@180°C
Hot Plate Gel Time 70 sec@150°C 45±15 sec@160°C 60 sec@180°C 60 sec@180°C
Edge Coverage, % 45 45 45 45
Hardness, shore D >80 >90 - -
Impact Resistance, cm >50 >50 >50 >50
Dielectric Strength (kV/mm) >42 >35 >35 >35
Flammability, UL94 V-0 V-0 V-0 V-0
Min. Coating Thickness 0.3mm 0.3mm 0.1mm 0.3mm
Max. Coating Thickness 1mm 1mm 2mm 3mm
Electrostatic Spray ■■■ ■■□ ■■■ ■■■
Dip Coating ■□□ ■■■ ■■■ ■■■
Available Color

●●●●●

●●

●●●●●

●

Preheat Temperature 180~240 °C 150~180 °C 180~230 °C 180~230 °C
Curing Conditions 200°C x 15min 200°C x 15min 200°C x 30min 200°C x 30min

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers