EPOCAST 1628

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EPOCAST 1628

Main features

  • Ultra Low Density Paste
  • Flame-Resistant Application Paste Material
  • Non-Sag Placement Control

Product Description

EPOCAST® 1628 A/B is a two-component, ultra-low-density epoxy syntactic supplied as a soft paste for reinforcing honeycomb structures. The mixed pale-yellow material has a typical density of 0.50 g/cc and an extrudable, non-sag consistency for filling honeycomb core sections and the edges of composite sandwich constructions with a putty knife or trowel. After cure, the material can be sanded and machined for finishing. The flame-retardant system is qualified to BMS 5-28, Type 28, for composite edge-reinforcement applications where lightweight construction and controlled paste placement are important.

Key features

  • Ultra-low-density system: The mixed epoxy syntactic has a typical density of 0.50 g/cc for lightweight honeycomb core and edge reinforcement.
  • Extrudable, non-sag paste: The material can be spread with a putty knife or trowel to fill core sections and composite sandwich edges.
  • Flame-retardant and qualified: Qualified to BMS 5-28, Type 28, with documented FAR 25.853 60-second vertical flammability results.

Applications / Suitable for

  • Edge reinforcing of honeycomb structures
  • Filling honeycomb core sections and edges of composite sandwich constructions
Product Family

EPOCAST 1628

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
Pale Yellow
Density (g)
0.50 g/cm3
Mix Ratio
100:25

Additional Information

Technical properties

As-supplied / before-processing properties

Typical values for the separate components and mixed system. These values are not product specifications.

Property Value Unit Method / condition
Color White / yellow / pale yellow — Visual; A resin / B hardener / mixed system
Density 0.45 / 0.52 / 0.50 g/cc ASTM D1622; A resin / B hardener / mixed system
Physical form and rheology Paste — ASTM D2196 at 25°C; A resin, B hardener and mixed system
Mix ratio 100:25 Parts by weight A resin:B hardener; mix thoroughly for several minutes
Gel time 65 min ASTM D2471; 60 g mixed system at 25°C
Typical cure schedule 48 h at 25°C; or gel at room temperature plus 5 h at 52°C — Material should be above 18°C during mixing
Technical properties

After-processing / final-state properties

Typical cured properties for evaluation purposes. Results depend on the stated test method, specimen and temperature and are not product specifications.

Property Value Unit Method / condition
Compressive strength 2,800 (19.3) psi (MPa) ASTM D695 at 25°C
Compressive strength 600 (4.1) psi (MPa) ASTM D695 at 82°C
Compressive strength 550 (3.8) psi (MPa) ASTM D695 at 121°C
Compressive modulus 230 (1.6) ksi (GPa) ASTM D695 at 25°C
Tensile lap shear strength 800 (5.5) psi (MPa) ASTM D1002; aluminum-to-aluminum at 25°C
Vertical flammability 0 s extinguish time; 0.3 in burn length — FAR 25.853; 60-second vertical test
Weight gain after immersion 1.5 / 2.5 / 3.5 / 3.4 % ASTM D543; 24 h at 25°C in Mil-S-3136 Type III fluid / Mil-M-5606 hydraulic fluid / Skydrol 500-A / distilled water, respectively