EPOCAST 1619-1

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EPOCAST 1619-1

Main features

  • Flame-Retardant Epoxy Syntactic
  • Room-Temperature Encapsulation Cure
  • Pourable/Extrudable Mixed Processing

Product Description

EPOCAST® 1619-1 A/B FR Epoxy Syntactic is a two-component, low-density, flame-retardant epoxy syntactic formulated for potting fasteners in honeycomb structures. The mixed off-white semi-paste has a density of ≤0.70 g/cm³ and can be poured or extruded through a 1/8 in. (3 mm) nozzle for placement in lightweight aerospace assemblies. It can be cured at room temperature or with a moderate elevated-temperature cycle and is qualified to Boeing BMS5-28, Type 19. The cured material resists water, fungus, and most aircraft fluids and provides documented insert pull-out and torque-out performance.

Key features

  • Low-density mixed system: Mixed density of ≤0.70 g/cm³ supports weight-sensitive honeycomb and aerospace structures.
  • Pourable and extrudable application: The mixed semi-paste delivers ≥250 g/min through a 1/8 in. nozzle under the BMS5-28 test method.
  • Aerospace-qualified flame resistance: Qualified to Boeing BMS5-28, Type 19, with a passing 12-second vertical-burn result and no dripping.
Product Family

EPOCAST 1619-1

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
Off-White
Density (g)
0.70 g/cm3
Mix Ratio
100:25
Physical Properties
Viscosity
400 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Typical as-supplied and processing data. Mix the resin and hardener for 3–5 minutes at 100:25 by weight. Remix the resin before use if filler separation occurs, and keep material above 18°C during mixing.

Property Value Unit Method / condition
Appearance A resin: off-white; B hardener: amber; mixed: off-white — Visual
Density A resin: 0.60; B hardener: 1.00; mixed: ≤0.70 g/cm³ ASTM D1622
Viscosity / consistency A resin: paste; B hardener: 400 cP; mixed: semi-paste — ASTM D2196 at 25°C
Mix ratio 100:25 Parts by weight A resin:B hardener
Extrudability ≥250 g/min BMS5-28; 1/8 in. nozzle
Gel time 20–40 min 62.5 g at 25°C
Typical cure cycles 7 days at 25°C; or gel at room temperature followed by 5 hours at 52°C — Typical cure schedules
Technical properties

After-processing / final-state properties

Typical cured-property data determined using the stated test methods and conditions. These values do not constitute product specifications or universal design allowables.

Property Value Unit Method / condition
Lap shear strength 1800 (12.4) psi (MPa) ASTM D1002; aluminum-to-aluminum at 23°C
Compressive strength at 23°C 7200 (49.7) psi (MPa) ASTM D695
Compressive strength at 82°C 480 (3.3) psi (MPa) ASTM D695
Flammability Pass; <1 s extinguishing time; <1.0 in. burn length; no drip — BMS5-28; 12-second vertical burn
Weight gain after fluid or water exposure <1.0 for each listed medium % wt. ASTM D543; 24 hours at 25°C in Mil-S-3136 Type III fluid, Mil-H-5606 hydraulic fluid, Skydrol 500A and distilled water
Hardness 65 Shore D ASTM D2240
Insert pull-out strength 400 (1782) lb (N) BMS5-28
Insert torque-out strength 110 (12.4) lbf-in (N·m) BMS5-28

Leading Brands Trust in Our Products and Services