LOCTITE ECCOBOND E1172A

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

Loctite Eccobond 50300HT

Main features

  • Void free Underfill
  • Fast cure at low temperature
  • Long pot life

Product Description

LOCTITE ECCOBOND E 1172 A monocomponent epoxy is formulated for use with very fine area array devices where SMT transparent processing is critical. This material can be used to under-fill devices with 25 micron geometries.

LOCTITE ECCOBOND E 1172 A provides a uniform and void-free underfill, maximizing the device's temperature cycling capability, distributing stress away from solder connects. It is a low CTE, non anhydride product with a long pot life. Thermal conductivity still needs TBD but it is around the 0.55 W/mK mark.

 

Cure Schedule

  • 6 minutes @ 135°C
  • 3 minutes @ 150°C
  • 30 minutes @ 100 °C plus 5 minutes @ 135 °C (low stress)
Product Family

ECCOBOND E1172A

1. Select Package Type
Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

Product availability
US Shipping in 35 days
CA Shipping in 12 weeks
EU Shipping in 20 days
Packaging
Please select Package Type.
TDS, SDS & Technical Documents

Technical Specifications

General Properties
Pot Life
48 hours
Thermal Properties
Glass Transition Temperature (Tg)
135 °C
Physical Properties
Viscosity
17,000 mPa.s

Additional Information

Testing underfills for Reflow reliability

Here are some anecdotal results from one of our active projects. Please note that these are not official Henkel reliability results but customer outcomes.

We compared 3 Types of underfill with the following curing schedules:

  • FP4531 30min@160°C
  • UF1173 30min@100°C+30min@135°C
  • E1172A  30min@100°C+30min@135°C

We prepared around 20 samples for each underfill. We exposed them to a the temperature profile of normal lead free reflow cycle and tested functionality to see after how many reflow cycles the samples start to fail.

  • FP4531 failed after the first cycle.
  • UF1173 failed after the 2nd cycle 
  • E1172 failed only after the 3rd cycle

 

 

ECCOBOND E 1172 A

ECCOBOND UF 1173

ECCOBOND FP4531

 

PASS

FAIL

PASS

FAIL

PASS

FAIL

1. Oven run

22

0

20

0

18

5

2. Oven run

22

0

19

1

-

-

3. Oven run

21

1

-

-

-

-

 

Does this make E 1172 the superior product and the other ones the inferior? Absolutely not.

These were tested under very specific customer conditions (note the different temperature of FP4531) and are just here to help you have a general outlook and some ballpark figures about these temperatures. These could turn on their heads if the process was different.

 

Do you have Outgassing properties for E1172A?

We do not have test data for outgassing on E1172A. However, we know that a related product with similar chemistry, E1173 has TML% = 0,43 and CVCM% = 0,02; so we are confident that E1172A can meet NASA/ESA outgassing requirements.

Leading Brands Trust in Our Products and Services