DOWSIL 93-076-2

Harmonization Code : 2901.10.00.00 | Acyclic hydrocarbons; Saturated

DOWSIL 93-076-2

Main features

  • Two-Hour Mixed Work Window
  • 680 psi Cured Tensile Strength
  • 10:1 Controlled Mixing

Product Description

DOWSIL 93-076-2 RF Sealant mixes at 10:1 by weight to create a high-viscosity, two-part silicone elastomer sealant that cures at room temperature. The catalyzed material has a two-hour working time at 25 deg C and an extrusion rate of 35 g/min after two hours, providing a defined application window for controlled bead placement. It sets up in 24 hours and reaches optimum physical properties in five days. After 24 hours at 25 deg C and 50% relative humidity, the sealant has 680 psi tensile strength, 120 ppi Die B tear strength and 350% elongation; Shore A hardness reaches 46 after five days.

Key features

  • 10:1 base-to-catalyst mix: Provides a defined two-part preparation ratio by weight.
  • Two-hour working time: Supports controlled application before viscosity build.
  • High cured strength: Typical tensile strength is 680 psi with 120 ppi Die B tear strength.

Applications

High-performance sealing applications using a two-part room-temperature-cure silicone elastomer.

Product Family

DOWSIL 93-076-2

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
Gray / Beige
Component System
Two (Sealant base / Catalyst)
Mix Ratio
10/1
Mechanical Properties
Elongation
400 %
Electrical Properties
Dielectric Strength
16 kV/mm
Volume Resistivity
1x10¹³ Ohms⋅cm

Additional Information

Technical properties

As-supplied / before-processing properties

Typical component and mixed-material properties. Values are not specifications.

Property Value Unit Method / condition
Base / curing-agent color Gray / turquoise As supplied
Mix ratio 10:1 Base to curing agent by weight
Working time 2 hr At 25 deg C
Extrusion rate 35 g/min Two hours after mixing; CTM0364
Set-up time 24 hr Room-temperature cure
Optimum property development 5 days Room-temperature cure
Shelf life 9 months At or below 32 deg C; original unopened containers
Technical properties

After-processing / final-state properties

Typical physical properties after 24 hours at 25 deg C and 50% relative humidity; hardness uses the five-day value.

Property Value Unit Method / condition
Durometer hardness 46 Shore A CTM0099 / ASTM D2240; five-day value
Tensile strength 680 psi CTM0137A / ASTM D412
Tear strength, Die B 120 ppi CTM0159A
Elongation at break 350 % After 24 hr at 25 deg C and 50% RH

Leading Brands Trust in Our Products and Services