ARALDITE 2013-1

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2013-1

Main features

  • Thixotropic Vertical-Surface Control
  • 80 to 90-Minute Working Window
  • 17 MPa Lap Shear

Product Description

ARALDITE® 2013-1 is a two-component, room-temperature-curing epoxy paste adhesive developed primarily for metal bonding and also suitable for ceramics, glass, rubbers, rigid plastics, and other commonly used materials. Its thixotropic, metal-colored paste supports vertical application and mixes at 100:60 by weight or 1:1 by volume. The mixed adhesive has a pot life of 80–90 minutes for a 100 g mass at 25°C, providing a practical assembly window. A 0.05–0.10 mm adhesive layer is recommended for greatest lap shear strength, with specified lap shear strength above 17 MPa at 23°C. The cured system combines high strength and toughness with documented environmental and chemical resistance.

Key features

  • Vertical-application paste: Thixotropic rheology supports application on vertical joint surfaces.
  • Controlled mixing and working time: Mixes 1:1 by volume and provides an 80–90 minute pot life for 100 g at 25°C.
  • Documented strength and resistance: Specified lap shear strength exceeds 17 MPa at 23°C, with documented environmental and chemical resistance.

Applications / Suitable for

  • Metal bonding
  • Ceramic and glass bonding
  • Rubber and rigid-plastic bonding
Product Family

ARALDITE 2013-1

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Pot Life
85 minutes
Specific Gravity
1.2
Physical Properties
Viscosity (Part A)
550000 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Component and mixed-material properties for ARALDITE® 2013-1. Preserve the stated component, quantity, temperature, and ratio basis when evaluating processing.

Property Value Unit Method / condition
Part A appearance Grey paste — Visual method A112; specified data
Part B appearance Beige paste — Visual method A112; specified data
Mixed appearance Grey paste — Visual method A112; specified data
Specific gravity A: ca. 1.4; B: ca. 0.9; mixed: ca. 1.2 — As supplied
Part A viscosity 380–720 Pa·s At 25°C
Part B and mixed rheology Thixotropic — At 25°C
Pot life 80–90 min 100 g mixed mass at 25°C
Mix ratio, A:B 100:60 by weight; 1:1 by volume — Bulk mixing or cartridge format
Technical properties

After-processing / final-state properties

Cured-property values are tied to the stated methods and cure conditions. Typical averages are technical information, not guaranteed design values.

Property Value Unit Method / condition
Lap shear strength >17 MPa At 23°C; method A501; specified data
Tensile strength 22 MPa ISO 527; cure 16 h at 40°C; tested at 23°C; typical average
Tensile modulus 1370 MPa ISO 527; cure 16 h at 40°C; tested at 23°C; typical average
Elongation at break 1.8 % ISO 527; cure 16 h at 40°C; tested at 23°C; typical average
Glass transition temperature 63.3 °C DMA; cure 16 h at 40°C; typical average