ABLESTIK 45LV

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ABLESTIK 45LV

Main features

  • Flexible Cured Adhesive
  • 16,000 to 30,000 mPa s Mixed Viscosity
  • 16 kV/mm Dielectric Strength

Product Description

LOCTITE® ABLESTIK 45 LV is a two-component, low-viscosity epoxy adhesive for general assembly bonding of metals, glass, and plastics, including dissimilar substrate combinations such as metal-to-plastic assemblies. Used with LOCTITE® CAT 15LV, the system supports rigid, semi-rigid, or flexible formulations through resin-to-hardener mix ratios of 100:25, 100:50, or 100:100 by weight. Mixed viscosity ranges from 16,000 to 30,000 mPa·s, depending on the selected formulation, with guideline room-temperature and accelerated heat-cure schedules. The cured formulations provide electrical insulation, thermal conductivity of 0.4 W/(m·K), and formulation-dependent mechanical flexibility and operating-temperature capability.

Key features

  • Variable cured flexibility: Rigid, semi-rigid, and flexible formulations are produced using documented 100:25, 100:50, and 100:100 resin-to-hardener ratios by weight.
  • Low-viscosity assembly bonding: Mixed viscosity ranges from 16,000 to 30,000 mPa·s, depending on formulation.
  • Room-temperature or heat cure: Guideline schedules range from 16 to 24 hours at 25°C to 30 to 60 minutes at 90°C.

Applications / Suitable for

  • General assembly bonding
  • Bonding metals, glass, and plastics
  • Bonding dissimilar substrates such as metal to plastic
  • Assemblies requiring rigid, semi-rigid, or flexible cured adhesive behavior
Product Family

ABLESTIK 45LV

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Chemistry Type
Epoxy
Physical Properties
Viscosity (Part A)
35000 mPa.s
Viscosity (Part B)
11000 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Typical component, mixed, handling, storage, and guideline cure information before final processing.

Property Value Unit Method / condition
Technology Epoxy — Two-component adhesive system
Appearance — resin Black liquid — Component A; TDS and resin SDS description
Appearance — hardener Black — Component B, LOCTITE CAT 15LV
Resin viscosity 35,000 mPa·s (cP) Part A; test method and temperature not stated
Resin specific gravity 1.58 — TDS value; resin SDS reports relative density of 1.6
Hardener viscosity 11,000 mPa·s (cP) LOCTITE CAT 15LV; test method and temperature not stated
Hardener specific gravity 0.97 — LOCTITE CAT 15LV
Mix ratio — rigid formulation 100:25 by weight Resin:LOCTITE CAT 15LV
Mixed viscosity — rigid formulation 30,000 mPa·s (cP) Test method and temperature not stated
Working time — rigid formulation 120 minutes 100 g mass at 25°C
Mix ratio — semi-rigid formulation 100:50 by weight Resin:LOCTITE CAT 15LV
Mixed viscosity — semi-rigid formulation 25,000 mPa·s (cP) Test method and temperature not stated
Working time — semi-rigid formulation 90 minutes 100 g mass at 25°C
Mix ratio — flexible formulation 100:100 by weight Resin:LOCTITE CAT 15LV
Mixed viscosity — flexible formulation 16,000 mPa·s (cP) Test method and temperature not stated
Working time — flexible formulation 90 minutes 100 g mass at 25°C
Resin shelf life 12 months At 25°C
Guideline cure schedules 16–24 hours, 4–6 hours, 2–4 hours, or 30–60 minutes — 16–24 hours at 25°C; 4–6 hours at 45°C; 2–4 hours at 65°C; or 30–60 minutes at 90°C
Technical properties

After-processing / final-state properties

Typical cured properties by formulation. Values depend on the selected resin-to-hardener ratio and are reference data rather than product specifications.

Property Rigid Semi-rigid Flexible Unit / method / condition
Operating-temperature range -40 to 90 -55 to 80 -55 to 65 °C; documented formulation ranges
Glass-transition temperature 68 38 21 °C; ISO 11357-2
Coefficient of thermal expansion — below Tg 55 63 80 ppm/°C; ASTM D3386
Coefficient of thermal expansion — above Tg 148 159 188 ppm/°C; ASTM D3386
Thermal conductivity 0.4 0.4 0.4 W/(m·K); test method and temperature not stated
Hardness 82 74 50 Shore D; ISO 868
Water absorption — 24 hours 0.1 0.2 1.7 %; ASTM D570
Dielectric breakdown strength 16 16 16 kV/mm; IEC 60243-1
Volume resistivity >1 × 1015 >1 × 1015 >1 × 1015 Ω·cm; IEC 60093
Aluminum lap shear strength at 25°C 17 (2,400) 16 (2,300) 7 (1,000) N/mm² (psi); ISO 4587
Aluminum lap shear strength at 65°C 9 (1,300) 3.5 (500) — N/mm² (psi); ISO 4587

Leading Brands Trust in Our Products and Services