3M 1357L

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

3M 1357L

Main features

  • Low-Viscosity Large-Area Application
  • Fast Ten-Minute Drying
  • Thirty-Minute Bonding Range

Product Description

3M Neoprene High Performance Contact Adhesive 1357L is a low-viscosity, one-part solvent-based neoprene contact adhesive for large-area and composite lamination. The gray/green liquid contains 17 to 19 wt% solids and has typical viscosity of 35 to 65 cP at 27 deg C, supporting spray, brush, or roller application. Applied to both prepared surfaces, it dries in about 10 minutes and provides an approximately 30-minute bonding range at 21 deg C and 35% RH. Uniform pressure develops immediate handling strength for machining or trimming after assembly. The adhesive bonds rubber, cloth, metal, wood, foamed glass, paper honeycomb, and decorative plastic laminates in supported industrial laminating and panel-construction work.

Key features

  • Low-viscosity application: Typical 35 to 65 cP viscosity at 27 deg C supports spray, brush, and roller coating.
  • Controlled bonding window: The adhesive dries in about 10 minutes and provides an approximately 30-minute bonding range at 21 deg C and 35% RH.
  • Immediate handling strength: Uniform assembly pressure supports machining or trimming directly after the bond is formed.

Applications

Applications include large-panel and composite lamination and bonding rubber, cloth, metal, wood, foamed glass, paper honeycomb, and decorative plastic laminates.

Product Family

3M 1357L

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
gray/green
Solids
17-19 %
Thermal Properties
Flash Point
-26 °C
Physical Properties
Viscosity
35-65 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

PropertyValueUnitMethod / condition
BasePolychloroprene-Typical
ColorGray / green-Typical
Solids content by weight17 to 19%Typical
Viscosity35 to 65cPBrookfield RVF #2 at 20 rpm and 27 deg C
Weight per gallon6.6 to 6.8lb/galTypical uncured material
Coverage219ft2/galAt 27 g/m2 dry
Flash point-26deg CTCC
Technical properties

Final-state / after-processing properties

PropertyValueUnitMethod / condition
180 deg peel adhesion256oz/inCanvas to steel; 24 h at 23 deg C
180 deg peel adhesion496oz/inCanvas to steel; 72 h at 23 deg C
180 deg peel adhesion296oz/inCanvas to steel; 3 weeks at 66 deg C
Overlap shear strength452psiBirch to birch; 2 weeks at 23 deg C
Overlap shear strength536psiBirch to birch; 3 weeks at 23 deg C
Overlap shear strength158psiBirch to birch; 3 weeks at 107 deg C